The control of the wall thickness of straight seam steel pipe is a difficult point in the production of steel pipes. At present, the methods of straight seam steel pipe manufacturers in the production of wall thickness accuracy generally include:

1. Tube billet heating: the heating should be uniform, and rapid temperature rise and fall are prohibited. The temperature of each rise and fall should be kept stable and slow, and the maximum rise and fall temperature should not exceed 30°C.
2. Rolling mandrel: Thick-walled tube and solid billet with uniform wall thickness can greatly reduce the probability of mandrel bending and deformation, and can effectively improve the wall thickness accuracy of the steel pipe.
3. Accuracy of the mandrel: The external machining accuracy of the mandrel is controlled at ±0.1mm, and the straightness direction of the mandrel does not exceed 5mm. When welding, a precision-machined pin is inserted between the two core rods for positioning, to avoid excessive deviation of the total straightness formed by welding.
4. Process: Determine whether the centering device is in place, adjust the center of the relevant core-holding rollers, the opening angle and the opening size of each movement are consistent, and the center of the core-holding rollers should be on the rolling line
5. Centering roller: advanced technology, avoiding the situation that the center is thinned and the wall thickness increases beyond the control limit, and the accuracy of the wall thickness is improved.
6. Perforated mandrel: The perforated mandrel generally chooses a thick-walled pipe with an outer diameter of Φ108mm-Φ114mm, a wall thickness of ≥25mm, and an average wall thickness.
7. Rolling middle line: ensure that the rolling middle line of the piercing machine is consistent with the middle line of the piercing trolley, avoid “up rolling” or “bottom rolling”, so that the tube blank can maintain uniform force when piercing.
8. Rolling tools: The worn-out plugs, guide plates, rolls, and other rolling tools should be replaced in time.
9. Rolling tool device: The center of the roll distance and guide distance must be on the rolling line. Ensure that the middle line of the guide distance and the roll distance is on the middle line of the piercing and rolling, that is, the upper and lower roller distances are equal, and the left and right guide distances are equal.

Straight seam steel pipe straightening method:
1. The straight seam steel pipe is bent in the same direction as the weld
Reason: Insufficient normalizing treatment of the weld seam, thermal stress exists on the side of the pipe near the weld seam, so it bends in one direction after cooling.
Solution: A. Adjust the middle roller to increase the deflection curve appropriately; B. Straighten twice; C. Temper the pipe as a whole when it cannot be straightened directly.
2. Straight seam steel pipe is bent irregularly
Reason: A. The pressure between the three rollers is inconsistent; B. The straightening roller wears a lot.
Solution: Check and adjust whether the upper straightening roller is loose, and use a sample stick to straighten the length of the contact line between the three lines.
3. The length of the straight seam steel pipe is greatly shortened
Reason: The rolling angle difference between the three straightening rollers is too large; the straightening pressure is relatively large.
Solution: Adjust the roller pressure angle to be as consistent as possible; properly adjust the straightening pressure.
4. One end of the straight seam steel pipe is bent
Cause: The distance between the rollers is too large.
Solution: Choose a straightening machine with a smaller spacing suitable for the corresponding pipe diameter.
5. The head of the straight seam steel pipe is not round
Reason: The contact phase between the three straightening rollers is improperly distributed or overlapped, and the roller pressure is too large.
Solution: Properly adjust the angle between the rollers and the pressure of the rollers on the pipe.

With the advancement and development of science and technology, many new technologies have been applied to steel pipe straightening machines. For example, the seven-roller type straightening machine was improved and applied by a certain company, the model is a 3-1-3 steel pipe straightening machine. It adopts a different structural form from the usual six-roller straightening machine and solves the problem of adjusting the straightening roller group in the circumferential direction. The characteristic is that the driving roller adjusts its height up and down by adjusting the inclined iron so that the three straightening rollers can be adjusted radially in the direction of 120° of the circumference, while the straightening center line remains unchanged. The advantage is that the structure is simple and easy to adjust, and the force on the circumference of the pipe to be corrected is uniform. Therefore, the straightening accuracy is high and good, and the applicable specification range is large.


Contact Us

Telephone:
+86-0731-8867-8530